Wrought Copper Alloys: Coppers (C10100 - C15999)

Standard Designation for Wrought Copper Alloys

Loading...

Print Download in PDF

Coppers (C10100 - C15999)

* = are alloys registered with the U.S. EPA as Antimicrobial.

Show/Hide Elements

NOTE: If table columns below get misaligned due to zoom or show/hide elements function, please Refresh this page (or press F5).

NOTE: To print this page, use Print button above for best results.

UNS # Cu Pb Zn Fe P Al Ag As B O Sb Te Other Named Elements Status
Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max% Min%Max%
C10100*
Oxygen-Free-Electronic OFE
99.99(1)(2)(3)0.00050.00010.00100.00030.00250.00050.00050.00040.0002active
C10200*
Oxygen-Free OF
99.95(4)(1)(5)0.0010active
C10300*
Oxygen-Free Copper OFXLP
99.95(5)(6)0.0010.005active
C10400*
Oxygen-Free with Ag OFS
99.95(1)(5)(4)0.027(7)0.0010active
C10500*
Oxygen-Free with Ag OFS
99.95(1)(5)(4)0.034(8)0.001active
C10700*
Oxygen-Free with Ag OFS
99.95(5)(4)(1)0.085(9)0.001active
C10800*
OFLP
99.95(6)(5)0.0050.012active
C10810
Oxygen-Free with Ca MOFC-GC
99.95(10)0.0010.001 Ca
0.010 Ca
active
C10850
Oxygen-Free with Mg MOFC-HR
99.95(11)(12)0.0010.002 Mg
0.013 Mg
active
C10900*
Oxygen-Free
99.99(5)0.001 Bi
inactive
03/11
C10910*99.95(12)(5)0.005active
C10920*99.90(5)0.02active
C10930*99.90(5)0.044(13)0.02active
C10940*99.90(5)0.085(9)0.02active
C11000*
Electrolytic Tough Pitch ETP
99.90(14)(12)(5)active
C11010*
Remelted High Conducivity RHC
99.90(5)(14)(12)active
C11020*
Fire-Refined High Conductivity FRHC
99.90(12)(14)(5)active
C11025*
Fire Refined High Conductivity FRHC
99.90(15)(16)(5)0.01500.04500.00800.00200.01500.00100.01000.04000.00500.0010active
C11030*
Chemically Refined Tough Pitch CRTP
99.90(5)(12)(14)active
C11040*99.90(17)(18)(12)0.00050.00100.00250.00050.01000.06500.00040.0002active
C11045*
ETP ETP
99.90(19)(5)0.00050.00100.00250.00050.01000.06500.00040.0002active
C11050
ETP-R
99.90(20)0.00050.00300.00250.00050.01000.06500.00040.0002active
C11080
Replaced by C13100
99.8(5)inactive
03/92
C11100*
Electronic Tough Pitch, Anneal Resistant ETP
99.90(21)(5)(12)active
C11300*
Tough Pitch with Ag STP
99.90(5)(14)(12)0.027(7)active
C11400*
Tough Pitch with Ag STP
99.90(14)(5)(12)0.034(8)active
C11500*
Tough Pitch with Ag STP
99.90(14)(12)(5)0.054(22)active
C11600*
Tough Pitch with Ag STP
99.90(12)(5)(14)0.085(9)active
C11700*99.9(5)(23)0.040.0040.02active
C11900*
Copper Alloy
99.93(5)0.0020.010inactive
02/73
C11904*
Copper Alloy
99.90(5)0.027(24)inactive
03/92
C11905*
Copper Alloy
99.90(5)0.034(8)inactive
03/92
C1190699.90 0.054inactive
C11907*
Copper Alloy
99.90(5)0.085(9)inactive
03/92
C12000*
Phosphorus-Deoxidized, Low Residual P DLP
99.90(5)0.0040.012active
C12100*
Phosphorus-Deoxidized, Low Residual P DLPS
99.90(5)0.0050.0120.014(25)active
C12200*
Phosphorus-Deoxidized, High Residual P DHP
99.9(26)(5)0.0150.040active
C12210*99.90(5)0.0150.025active
C12220*99.9(5)0.0400.065active
C12300*
Phosphorus-Deoxidized, High Residual P DHPS
99.90(5)0.0150.0400.014(25)active
C12500*
Fire-Refined Tough Pitch FRTP
99.88(5)0.0040.0120.0030.025(27)0.050 Ni
0.003 Bi
active
C12510*99.9(5)0.0200.0800.050.030.0030.025(27)0.05 Sn
0.050 Ni
0.005 Bi
active
C1260099.5(5)0.200.40active
C12700*
Copper Alloy
99.88(5)0.0040.027(24)0.0120.0030.025(27)0.050 Ni
0.003 Bi
inactive
03/92
C12800*
Copper Alloy
99.76(5)0.0040.034(8)0.0120.0030.025(27)0.050 Ni
0.003 Bi
inactive
03/92
C12900*
Fire-Refined Tough Pitch with Ag FRSTP
99.88(5)0.0040.054(22)0.0120.0030.025(28)0.050 Ni
0.003 Bi
active
C13000
Copper Alloy
99.88(5)0.0040.085(9)0.0120.0030.025(27)0.05 Ni
0.003 Bi
inactive
03/92
C13100*99.8(5)active
C13150*
Copper
99.5(5)active
C13400*
Copper Alloy
99.99(5)0.00050.027(24)inactive
12/72
C13500*
Copper Alloy
99.99(5)0.00050.034(8)inactive
12/72
C13600*
Copper Alloy
99.99(5)0.00050.054(22)inactive
12/72
C13700*
Copper Alloy
99.99(5)0.00050.085(9)inactive
12/72
C14100
Copper Alloy
99.40(5)0.150.50inactive
07/74
C14180*99.90(5)0.020.0750.01active
C14181*99.90(5)0.0020.0020.0020.005 C
0.002 Cd
active
C14200*
Phosphorus-Deoxidized, Arsenical DPA
99.4(5)0.0150.0400.150.50active
C14210*
Copper Alloy
99.20(5)0.0130.0500.300.50inactive
03/92
C14300*
Cadmium Copper, Deoxidized
99.90(5)(29)0.05 Cd
0.15 Cd
active
C14310*
Cadmium Copper
99.90(5)(29)0.10 Cd
0.30 Cd
inactive
03/92
C14400*
Copper Alloy
99.90(5)0.050.030.0130.0250.0030.020.10 Sn
0.20 Sn
0.05 Ni
inactive
03/92
C14410*99.90(30)(5)0.050.050.0050.0200.10 Sn
0.20 Sn
active
C14415*99.96(30)0.10 Sn
0.15 Sn
active
C14420*99.90(5)(31)0.0050.050.04 Sn
0.15 Sn
active
C14425
Copper Copper
99.97(32)(5)0.100.100.0200.0100.25 Sn
0.35 Sn
0.020 Ni(33)
active
C14430*
Copper Alloy
Rem(5)0.25 Sn
0.35 Sn
inactive
03/92
C1443599.4(34)0.0010.30 Sn
0.60 Sn
active
C14440*
Copper Alloy
99.96(5)0.005 Sn
0.01 Sn
inactive
03/92
C14500*
Tellurium-Bearing PTE
99.90(35)(36)(5)0.0040.0120.400.7active
C1450599.8(37)0.0030.0010.100.50active
C14510*
Tellurium-Bearing
99.85(35)(5)0.050.0100.0300.300.7active
C14520*
Phosphorus-Deoxidized,Tellurium-Bearing DPTE
99.90(35)(5)0.0040.0200.400.7active
C14530*99.90(38)0.0010.0100.003(39)0.0230.003 Sn
0.023 Sn
active
C14700*
Sulfur-Bearing
99.90(5)(40)(36)0.002(40)0.0050.20 S
0.50 S(40)
active
C14710*
Copper Alloy
99.90(36)(41)0.05(41)0.010(41)0.0300.05 S
0.15 S(41)
inactive
03/92
C14720
Copper Alloy
99.50(40)(36)(5)0.10.0100.030(40)0.20 S(40)
0.50 S
inactive
03/92
C14730
Sulfur Bearing Copper
99.80(5)inactive
03/92
C14750*
High Copper Alloy
Rem(5)(42)0.0120.05 Mn
0.20 S
0.50 Mn
0.50 S
active
C15000*
Zirconium Copper
Rem(5)(37)0.10 Zr
0.20 Zr
active
C15100*99.80(37)(5)0.05 Zr
0.15 Zr
active
C15150*99.90(5)0.015 Zr
0.030 Zr
active
C15500*99.75(5)0.0400.0800.0270.10(24)0.08 Mg
0.13 Mg
active
C15600*
Copper Alloy
99.6(5)0.060.090.20 Co
0.30 Co
0.02 Mg
active
C15630Rem(10)0.0150.0400.60 Ni
0.90 Ni
active
C15650*
MA5J Copper
99.9(5)0.0150.0400.04 Co
0.06 Co
active
C15710*
Copper Alloy
99.71(5)0.010.010.080.120.070.15inactive
03/92
C15715*
Dispersion Strengthened Alloy
99.62(5)0.010.010.130.17(43)0.12(43)0.19active
C15720*
Dispersion Strengthned Alloy
99.52(5)0.010.010.18(43)0.220.160.24(43)active
C15725*
Dispersion Strengthened Alloy
99.43(5)0.010.010.23(43)0.270.20(43)0.28active
C15730*
Copper Alloy
98.94(5)0.040.260.34(43)0.220.32(43)0.46active
C15735*
Copper Alloy
99.24(5)0.010.010.330.370.290.37inactive
03/92
C15750*
Dispersion Strengthened Copper C3/60
98.56(5)0.040.42(43)0.500.220.520.68(43)active
C15760*
Dispersion Strengthened Alloy
98.77(5)0.010.010.58(43)0.620.520.59(43)active
C15780*
Copper Alloy
98.10(5)0.040.66(43)0.740.220.76(43)0.90active
C15790*
Copper Alloy
97.68(5)0.040.88(43)0.960.220.96(43)1.10active
C15815*
Dispersion Strengthened Alloy
97.82(5)0.010.010.130.17(43)1.21.80.19(43)active
C15900*
Dispersion Strengthened Coper C3/11
97.51(5)0.040.760.84(43)0.40(43)0.540.27 C
0.66 Ti
0.33 C
0.74 Ti
active

* = are alloys registered with the U.S. EPA as Antimicrobial.

(1) = This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS except for Alloy C10100 which has a minimum conductivity of 101% IACS.
(2) = Cu is determined by the difference between the impurity total and 100 %. For alloy C10100 the Cu value is exclusive of Ag.
(3) = The following additional impurity maximum limits shall apply: Bi 1ppm (0.0001%); Cd 1ppm (0.0001%); Mn 0.5ppm (0.00005%); Ni 10ppm (0.0010%); Se 3ppm (0.0003%); S 15ppm (0.0015%); Sn 2ppm (0.0002).
(4) = Cu is determined by the difference between the impurity total and 100%.
(5) = Cu value includes Ag.
(6) = Includes P.
(7) = Ag 0.027% min is the equivalent of, Ag 8 Troy Oz min.
(8) = Ag 0.034% min is the equivelant of, Ag 10 Troy Oz min.
(9) = Ag 0.085% min is the equivelant of, Ag 25 Troy Oz min.
(10) = Cu + Sum of Named Elements 99.5% min.
(11) = Cu + Sum of Named Elements, 99.95% min.
(12) = This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS.
(13) = Ag 0.044% min is the equivelant of, Ag 13 Troy Oz min.
(14) = Oxygen and trace elements may vary depending on the process.
(15) = The following additional maximum limits shall apply: Se 10 ppm (0.0010%); Bi 5 ppm (0.0005%); Sn 150 ppm (0.0150%); Ni 150 ppm (0.0150%); S 20 ppm (0.0020%); Cd 100 ppm (0.0100%).
(16) = The total maximum allowable of named elements is 750 ppm (0.0750%) not including oxygen.
(17) = Cu value is exclusive of Ag
(18) = The following additional maximum limits shall apply: Se 2ppm (0.0002%); Bi 1.0ppm (0.00010%); Group Total Te + Se +Bi 3ppm(0.0003%); Sn 5ppm (0.0005%); Ni 10ppm (0.0010%); S 15ppm (0.0015%). The total maximum allowable of named elements is 65 ppm (0.0065%) - does not include oxygen.
(19) = These total maximum limits shall apply; Se 2ppm(0.0002%); Bi 0.5ppm (0.00005%); Sn 5 ppm (0.0005%); Ni 10ppm (0.0010%); S 15 ppm (0.0015%).
(20) = The following additional impurity maximum limits shall apply: Bi 1 ppm (0.0015%); Ni 15 ppm (0.0015%); S 15 ppm (0.0015%); Se 2 ppm (0.0002%); Sn 15 ppm (0.0015%);
(21) = Small amounts of Cd or other elements may be added by agreement to improve the resistance to softening at elevated temperatures.
(22) = Ag 0.054% min is the equivelant of, Ag 16 Troy Oz min.
(23) = Includes B + P.
(24) = Ag 0.027 - 0.10% min is the equivalent of, Ag 8 - 30 Troy Oz min.
(25) = Ag 0.014% min is the equivalent of, Ag 4 Troy Oz min.
(26) = This includes oxygen-free Cu which contains P in an amount agreed upon.
(27) = 0.025 Te + Se.
(28) = Includes Te + Se.
(29) = Includes Cd. Deoxidized with Li or other suitable elements as agreed upon.
(30) = Includes Cu + Ag + Sn.
(31) = Includes Te + Sn.
(32) = Cu + Sum of Named Elements, 99.97% Min.
(33) = Includes Co.
(34) = Cu + Sum of Named Elements 99.7% min.
(35) = Includes Te + P.
(36) = Includes oxygen-free or deoxidized grades with deoxidizers (such as phosphorus boron lithium or others in an amount agreed upon.
(37) = Cu + Sum of Named Elements 99.9% min.
(38) = Includes Ag + Sn + Te + Se
(39) = Tellurium and/or Selenium
(40) = Includes Cu + S + P.
(41) = Includes Ag, S, P, and Pb
(42) = Cu + Sum of Named Elements 99.8% min.
(43) = All aluminum present as Al2O3; 0.04% oxygen present as Cu2O with a negligible amount in solid solution with copper.